Марки нержавеющей стали для крепежа: полное руководство по материалам для инженера

Stainless Steel Grades

Stainless Steel Families Used in Fasteners

Stainless steels are a family of iron–chromium alloys. Five stainless steel families appear in fasteners, each behaving differently under load and in corrosive service. The stainless steel grades for болты и винты you’ll specify most often come from these five families.

Austenitic (300 series: 201, 302, 303, 304, 316, 321, 347)

Austenitic grades are the workhorses. They contain 16–26% chromium and 6–14% nickel, stabilizing the face-centered cubic (FCC) austenite phase at room temperature. What that buys you is corrosion resistance, decent ductility, and strength you get from cold work rather than heat treatment.

  • 304(А2) is the default general-purpose grade: 18–20% Cr, 8–10.5% Ni, no molybdenum.

  • 316 (А4) adds 2–3% molybdenum for chloride resistance.

  • 321, 347, 303 cover high-temperature (Ti/Nb-stabilized) and free-machining (sulfur-added) needs.

  • 201 trades nickel for manganese to cut cost but is not a 304 substitute in demanding service.

Martensitic (410, 416, 420, 440C)

Martensitic grades (11.5–18% Cr, low nickel) harden by quenching and tempering like carbon steel. That makes them the choice when hardness and wear resistance matter more than corrosion: саморезы, set screws, машинные винты in mild environments. They are magnetic and noticeably less corrosion-resistant than 304.

Ferritic (430, 434)

Ferritic stainless (10.5–27% Cr, little nickel) is ferromagnetic and moderate in corrosion resistance. In fasteners it appears in cost-sensitive, mildly corrosive applications such as architectural trim, but it is seldom specified for structural stainless bolts. One procurement note worth flagging: because ferritic grades carry almost no nickel, their price is far less exposed to Ni-market volatility than 304/316. That is a legitimate reason to choose ferritic where the environment allows — not just a corrosion decision.

Duplex (2205, 2507)

Duplex grades split their microstructure roughly 50/50 between austenite and ferrite. So a duplex fastener gives you roughly double the yield strength of 316. That same hybrid also lifts pitting resistance to PREN 30–35 (2205) and 38–42 (super-duplex 2507). They dominate offshore, desalination, and subsea service where 316 would be marginal.

Precipitation-Hardening (17-4 PH, 17-7 PH)

PH grades combine a martensitic base with an aging heat treatment that precipitates copper- or nickel-rich phases for very high strength. 17-4 PH (Grade 630) reaches 1,310–1,380 MPa tensile in the H900 condition, far above any austenitic fastener, while keeping better corrosion resistance than 410. Aerospace, medical, and high-performance mechanical assemblies use them where strength-to-size is critical.

For a side-by-side look at how these families compare on strength, corrosion, and cost, see our stainless steel family comparison.

How Stainless Steel Resists Corrosion (The Passive Layer)

The word “stainless” is a misnomer. Stainless steels do corrode. They carry a built-in defense ordinary steel lacks: a passive film. Understanding it explains almost every grade decision that follows.

The chromium oxide film (1–3 nm, self-healing)

When chromium exceeds roughly 10.5%, the alloy spontaneously forms a nanoscopic layer of chromium oxide (Cr₂O₃). This film is only 1–3 nm thick. Invisible, but dense, adherent, and self-healing. If you scratch it, oxygen rebuilds it within milliseconds.

The catch: the film needs oxygen. In oxygen-starved crevices or where aggressive ions overwhelm it, protection fails locally, which is where grade selection becomes decisive.

Four alloying elements that decide performance

  • Chromium (Cr) builds the passive film. More Cr means broader environmental tolerance.

  • Molybdenum (Mo) sharply improves resistance to pitting and crevice corrosion in the presence of chlorides (salt). This is the single biggest difference between 304 and 316.

  • Nickel (Ni) stabilises the austenitic structure, giving high formability and weldability. Low-nickel grades (ferritic/martensitic) trade some corrosion breadth for cost and hardenability.

  • Nitrogen (N), added to duplex grades, raises both strength and PREN.

Two more practical points. First, surface finish counts: a smoother finish (e.g., bright-annealed or 2B) resists fouling and corrosion better than a rough one, because deposits are harder to trap. Second, passivation to ASTM A967 (nitric or citric acid) removes free iron picked up during machining and thickens the protective film — a sensible step for critical assemblies.

Pitting, crevice & tea-staining: three failure modes

  • Pitting starts when chloride ions (Cl⁻) punch through the passive film at a weak point: an inclusion, a scratch, a weld. Once a pit nucleates, the trapped chemistry turns acidic and eats inward, sometimes to failure in weeks.

  • Crevice corrosion is pitting’s cousin. It strikes under washers, in thread roots, and beneath gaskets where stagnant solution and low oxygen let the film collapse. It is the most common “mystery” failure on otherwise good stainless.

  • Tea staining is the mild, cosmetic end: a brown surface discoloration from iron contamination or shallow attack. It looks alarming but rarely threatens structure, though it signals the environment is at the edge of what the grade can handle. See why stainless steel fasteners still rust

Real-world scenario: A coastal wastewater plant specified 304 (A2) hex bolts on handrail assemblies 800 m from the shoreline. Within 14 months the bolts showed tea staining and the first pits. The fix was switching to 316 (A4); the 304 had done exactly what its chemistry permitted, and the spec had asked for more.

PREN and what it tells you about chloride resistance

The Pitting Resistance Equivalent Number (PREN) is the engineer’s shorthand for chloride resistance:

PREN = %Cr + 3,3 × %Mo + 16 × %N

Higher is better. Typical values: 304 ≈ 18–19, 316 ≈ 24–26, Duplex 2205 ≈ 30–35, super-duplex 2507 ≈ 38–42.

PREN explains the key fact: 316 resists chlorides roughly an order of magnitude better than 304. Field data puts 304 pitting onset near ~300 ppm chloride, while 316 holds to ~1,000–2,000 ppm.

For the full failure-mode breakdown: stress-corrosion cracking and intergranular attack, browse our Resources library on stainless steel corrosion mechanisms.

Крепежные изделия из нержавеющей стали

The Core Grades: 304 (A2) vs 316 (A4) for Fasteners

When it comes to stainless steel grades for fasteners, remember this above all: 304 and 316 are chosen for corrosion, not strength. Their mechanical properties are nearly identical. The molybdenum in 316 is the entire story.

Состав & property-class difference (A2-70, A4-70/80)

Элемент304 / A2316 / A4
Chromium (Cr)18.0–20.0%16.0–18.0%
Nickel (Ni)8.0–10.5%10.0–14.0%
Molybdenum (Mo)Никто2.0–3.0%
Carbon (C), max0.08%0.08%
PREN (typical)~18–19~24–26

In the ISO 3506 system, “A2” means austenitic grade 2 (the 304-family) and “А4” means austenitic grade 4. The dash number is the property class: a strength rating, not a corrosion rating:

  • А2-70/А4-70: minimum tensile 700 MPa, 0.2% proof stress 450 MPa.

  • А4-80: minimum tensile 800 MPa, proof stress 600 MPa (tighter composition, more cold work).

So “А4-80” means a 316-family alloy at the 800-MPa strength class. It is нет “more corrosion-resistant than A4-70”: just stronger.

Side-by-side comparison table

Атрибут304(А2)316 (А4)
Tensile strength (class 70)≥ 700 MPa≥ 700 MPa
0.2% proof stress (class 70)≥ 450 MPa≥ 450 MPa
Chloride pitting threshold (ambient)~300 ppm~1,000–2,000 ppm
ДРЕВЕСИНА~18–19~24–26
Magnetism (annealed)Essentially none*Essentially none*
Relative material cost1.00× (baseline)+15–25%
Best useIndoor, rural, mild urbanCoastal, marine, chemical, de-icing salt

*Cold heading and thread rolling can induce weak magnetism even in austenitic grades (see Section 4).

The numbers show why “pay for 316 for strength?” is the wrong question. You pay for 316 for среда, accepting the premium as insurance against chloride-driven failure.

Is 316 worth the 15–25% premium? (TCO framing)

A piecemeal view says 316 costs 15–25% more than 304, so use 304 wherever possible. A total-cost-of-ownership (TCO) view asks a different question: what does a failure cost?

Consider a coastal walkway: 304 bolts at $1.00, 316 at $1.20. If the 304 needs replacement at year 8, plus labor and access, the savings evaporate. In chloride service, 316 typically pays back its premium within 3–5 years by avoiding one premature intervention. The decision is therefore economic, and the answer usually favors 316 wherever chlorides are present.

Real-world scenario — food processing: A dairy plant specified 304L for its stainless equipment frames. Indoors and regularly wash-down cleaned, 304L delivered years of maintenance-free service at the lowest alloy cost. When the same frames were later extended to an outdoor loading bay near a salted road, pitting appeared within 18 months — the grade, not the maintenance, was the limit.

Real-world scenario — offshore access platform: A North Sea maintenance walkway originally used 304 hardware. Within two seasons, bolt heads showed red rust and crevice pitting at the splash line. Re-specified to A4-80 (316L), with duplex 2205 in the submerged members, the same joints ran five years with only cosmetic inspection. The molybdenum content — not a higher strength class — was what changed the outcome.

For the exhaustive cost-and-performance model, see our 304 vs 316 stainless steel fasteners comparison. For payback math, see is 316 stainless steel worth the cost.

Mechanical & Physical Properties by Grade (data table)

The table below consolidates representative minimum values from ISO 3506-1 (metric) and ASTM F593 (inch-series PH). For full property ranges, see typical mechanical properties of 316 stainless.

Tensile / yield / hardness by grade & property class

Grade (family)Класс недвижимостиMin. tensile (MPa)Min. 0.2% proof/yield (MPa)Magnetic?Типичное использование
A2 (304, austenitic)70700450Weakly, if cold-workedGeneral purpose
A4 (316, austenitic)70700450Weakly, if cold-workedМорская, химическая
A4 (316, austenitic)80800600Weakly, if cold-workedHigh-load chloride service
C1 (410, martensitic)70700410ДаHard, mildly corrosive
17-4 PH (Grade 630)H9001,310–1,3801,170–1,250ДаAerospace, high strength
17-4 PH (Grade 630)H1150860–930725–860ДаHigh strength, less hard
Дуплекс 2205100≥ 1,000≥ 800Yes (ferritic phase)Offshore, subsea, desalination

Two things stand out. First, austenitic fasteners top out near 800 MPa (class 80); if you need more, you leave the austenitic family for martensitic, PH, or duplex. Second, strength and corrosion resistance trade off across families: 410 is hard but corrosion-limited, while 316 is corrosion-proof but strength-limited without cold work.

Magnetic behavior myth-busting (cold-work induced magnetism)

“If it sticks to a magnet, it isn’t stainless.” This is the most repeated and most wrong rule on the shop floor.

Austenitic 304/316 are non-magnetic in the fully annealed state because their FCC structure has no net magnetic moment. But cold heading and thread rolling plastically deform the metal, partially transforming some austenite into strain-induced martensite. That transformed layer is magnetic. A perfectly genuine A2-70 bolt will often cling to a magnet simply because it was cold-formed.

An incoming inspector once rejected A2-70 socket-head capscrews as “counterfeit carbon steel” because they stuck to his magnet. The right test for “is this the right grade?” is a PMI analyzer or chemistry check, never a magnet.

How крепеж из нержавеющей стали Are Made (Manufacturing Process)

Как изготавливаются крепежи из нержавеющей стали

Most guides stop at “pick a grade.” They skip the question a procurement engineer should ask: how was this part actually made? Manufacturing controls the properties you can’t see: grain flow, surface integrity, and the health of the passive film.

Wire drawing & annealing

Production begins with stainless wire rod. The rod is drawn through hardened dies to the precise diameter the fastener requires. Drawing work-hardens the wire and reduces ductility, so it is annealed in a controlled (often low-oxygen) atmosphere furnace to restore the softness needed for forming. Get the atmosphere wrong and the surface oxidizes, compromising the passive layer itself.

Холодный заголовок & thread rolling

The cut wire blank is forged into shape by a high-speed cold heading machine at room temperature. Cold heading beats machining because the grain flow follows the fastener shape, improving fatigue strength and eliminating waste.

Threads are almost always formed by thread rolling, not cutting. Hardened dies displace material to raise the thread form, leaving compressive residual stresses at the root that resist crack initiation. Rolled threads outperform cut threads in fatigue and finish.

Heat treatment (martensitic / PH grades)

Austenitic 304/316 are not quench-hardened; their strength comes from cold work, and heavily deformed parts may receive a solution anneal (≈1,050–1,150 °C). Martensitic (410) and PH (17-4 PH) grades, by contrast, are hardened by quench-and-temper or aging cycles.

Passivation, pickling & surface finish (Ra)

Every forming step can smear free iron from tooling onto the surface. Left in place, that iron rusts and stains the part. Passivation re-establishes a dense, uniform passive film. Per ASTM A967 / AMS 2700, it means immersing the part in nitric or citric acid, which dissolves that free iron. Surface roughness (Ra) also matters: smoother finishes resist crevice attack better than rough ones.

Standards exist so “А4-80” means the same thing everywhere. Three frameworks matter.

Reading A2-70 / A4-80

Per ISO 3506-1 standard (the 2020 edition adds 6%Mo austenitic and duplex grades, plus a “100” property class), the designation breaks down as:

  • Letter = steel group: A = austenitic, C = martensitic, F = ferritic, D = duplex.

  • Digit = grade within the group: A1–A5 (A2≈304, A4≈316 with Mo; A5 is a stabilized 316 variant).

  • Dash number = property class: 50, 70, 80 (and 100 for duplex), corresponding to minimum tensile strength in hundreds of MPa.

Bolts are normally marked on the head with the class; always confirm the marking matches the spec. See what A2-70 and A4-80 mean.

АСТМ & DIN equivalents

For inch-series stainless fasteners, АСТМ Ф593 covers bolts, hex capscrews, and studs (including Grade 630 = 17-4 PH), with F594 for nuts and F738 for metric stainless. АСТМ А193/А320 cover high-temperature and low-temperature alloy-steel and stainless bolting for pressure equipment (B8 = 304, B8M = 316). ОТ specs (933/931, 934, 125) align with the ISO property-class system; “A4-80 DIN 933” is simply the ISO grade-and-class in DIN form. ЕН 10204 3.1 Mill Test Certificates (MTC) document actual heat analysis and mechanical results for traceability.

Selecting the Right Stainless Steel Grade for Fasteners

Selecting the right stainless steel grades for fasteners is ultimately an environmental decision. Map the service condition to a grade, then confirm strength with the property class. For a head-to-head against carbon and alloy steel, see our stainless vs carbon steel fasteners сравнение.

Применение винтов из нержавеющей стали

Quick selection by application

Environment / dutyRecommended gradeПочему
Indoor, dry, mild outdoor304 / 304L (A2)Cost-effective; enough corrosion margin
Marine, coastal, pool, de-icing salt316L (A4-70/80)Mo resists chloride pitting
Submerged / splash / high strength in seawaterДуплекс 2205PREN 34–36 + 2× yield strength
Chemical & petrochemical (mild)316L (A4)Broad chemical resistance
Chemical, warm chlorides, high stressДуплекс 2205SCC and pitting resistance
Food & pharmaceutical304L / 316LHygienic, weldable, easy to clean
High temperature (≤650 °C), mild env.410 (heat-treated)Hardenable strength + heat resistance
High-temp process (ASTM pressure equip.)A193 B8 / B8M (304/316)Specified for high-temp bolting
Decorative / budget / mild430 (F1)Low-nickel cost stability
Strength / wear, dry410 / 431Hardenable, high strength

Indoor / general-purpose → 304 (A2)

Dry interiors and mild urban atmospheres with no chlorides are 304 territory: furniture hardware, interior HVAC brackets, equipment never exposed to salt or chemical. It is the cost-optimal default.

Coastal / marine / chemical → 316 (A4)

Anything within splash zone of seawater, within a few kilometers of the coast, exposed to de-icing salts, or in contact with process chemicals should be 316. This includes marine hardware, coastal façades, food and pharmaceutical plants, and bridge expansion joints in cold climates.

Watch-out: Austenitic grades are vulnerable to chloride stress-corrosion cracking (SCC) above roughly 60 °C in the presence of chlorides. For hot, chloride-rich, high-stress duty, move to duplex 2205.

High-strength → 410 / 17-4 PH / Duplex 2205

When the limiting factor is load rather than corrosion:

  • 410 for hardness/wear in mildly corrosive settings (self-tapping, set screws).

  • 17-4 PH where very high strength is required and corrosion is moderate (aerospace, precision mechanisms).

  • Дуплекс 2205 where you need both high strength и serious chloride resistance (offshore, desalination, subsea).

Real-world scenario — self-drilling roof screws: A metal-building manufacturer needed screws that could drill their own hole and hold high clamp load. Austenitic 304 could not reach the required hardness; 410 (heat-treated) delivered the wear resistance and torque strength. Specified only for inland, atmospheric duty — the same screw would have rusted on a coastal roof.

Real-world scenario — seawater pump station: A desalination intake used 316 bolts that suffered crevice corrosion at bolt–flange interfaces within three years. Switching to duplex 2205 raised PREN from ~25 to ~35 and doubled joint strength, extending the maintenance interval beyond the project’s design horizon.

Specifier’s decision checklist (flowchart)

START
│
├─ Chlorides present (coastal air, de-icing salt, seawater, process chemicals)?
│ ├─ YES ──> Very high strength (>800 MPa) also required?
│ │ ├─ YES ──> Duplex 2205 (class 100) or 17-4 PH
│ │ └─ NO ──> 316 / A4 (class 70, or 80 if higher load)
│ └─ NO ───> High hardness / wear resistance required?
│ ├─ YES ──> 410 (C1) or 17-4 PH
│ └─ NO ──> 304 / A2 (class 70, or 80 if higher load)
│
├─ Confirm property class meets design tensile/proof load.
├─ Confirm galvanic compatibility with joined materials (Section 8).
└─ Specify passivation + finish (Ra) for demanding service.

Common Mistakes & Galvanic Compatibility

Even the right grade fails if it is joined wrong. These are the errors we see most often in the field.

8 spec errors that cause field failures

  1. Specifying 304 in a coastal or de-icing environment. The most common error; PREN ~19 cannot hold against chlorides.

  2. Assuming “stainless” means “non-magnetic” and rejecting good parts (Section 4), or accepting magnetic counterfeit.

  3. Ignoring crevices. Even 316 pits under a trapped washer in stagnant brine. Specify sealed joints or non-absorbing isolators.

  4. Over-specifying 316 where 304 suffices, inflating cost with no service benefit in benign interiors.

  5. Forgetting the galvanic partner. A perfect 316 bolt can destroy an aluminum frame (below).

  6. Thread galling. Austenitic stainless can cold-weld under high assembly torque, seizing the joint before the target clamp load is reached. Mitigate with proper lubrication, controlled torque, avoiding over-tightening, and pairing a harder nut with the bolt.

  7. Chloride stress-corrosion cracking (SCC). 304 and 316 are vulnerable above ~60 °C when chlorides and tensile stress coexist. If the service environment is hot and chloride-rich, specify duplex or a higher alloy from the start.

  8. Sensitization / weld decay. When carbon at weld zones precipitates chromium carbide, the adjacent area loses corrosion resistance. Always use low-carbon “л” grades (304L, 316L) for welded assemblies.

Dissimilar-metal rule (0.25 V, isolating washers)

Galvanic corrosion needs three things at once: two dissimilar metals, electrical contact, and an electrolyte (moisture, salt spray, even humid air).

Follow a simple rule: keep the potential gap between coupled metals under ~0.25 V on the galvanic series. Past that point, the more “active” (anodic) metal sacrifices itself to protect the “noble” (cathodic) one. Stainless in its passive state is noble. So when you bolt it into aluminum or plain carbon steel, the other metal corrodes, not the stainless.

Real-world scenario — rooftop HVAC on a coastal hospital: A contractor used A4-80 stainless bolts to secure an aluminum structural frame, assuming “all stainless, all safe.” Within two seasons the aluminum pitted and chalked at every joint. The fix was dielectric isolation: nylon sleeves and washers breaking the conductive path, plus a film of dielectric grease on the threads.

Two more principles save assemblies:

  • Mind the area ratio. A small anode against a large cathode fails fast (aluminum rivets in a stainless panel = disaster); a small noble fastener in a large anodic structure is tolerable.

  • Isolate deliberately. Nylon, neoprene, or glass-reinforced-epoxy sleeves and washers, full coatings on both surfaces, or a sacrificial zinc anode all work. When two metals far apart on the series must meet, assume you need a deliberate break between them.

Where stainless meets galvanized steel, the zinc is the sacrificial anode and protects the steel substrate. Ensure drainage so electrolyte doesn’t pool.

Quick Reference & Часто задаваемые вопросы

What does A2-70 mean?

A2-70 is a grade-plus-strength code stamped on stainless fasteners. A2 identifies the austenitic 304-family stainless; 70 is the property class, meaning a minimum tensile strength of 700 MPa and 0.2% proof stress of 450 MPa. It rates strength, not corrosion resistance.

Is stainless steel magnetic?

In the fully annealed state, austenitic 304/316 are essentially non-magnetic. But cold heading and thread rolling induce measurable magnetism, so a formed bolt may attract a magnet. Martensitic (410), PH (17-4), ferritic (430), and duplex grades are magnetic. A magnet can’t confirm grade. Only chemistry can.

Will 304 rust near the coast?

Yes, eventually. At ~300 ppm chloride (typical of coastal air and salt spray), 304 begins to pit and tea-stain. Within a few kilometers of the shore or where de-icing salts land, specify 316 for the chloride exposure.

Is 316 worth the cost?

In benign interiors, no: 304 is the economic choice. In chloride-exposed service, yes: the 15–25% premium typically pays back within 3–5 years by preventing one premature failure. Use a total-cost-of-ownership view, not unit price.

Can I use stainless with galvanized steel?

Cautiously. Zinc is anodic to passive stainless, so the galvanized coating sacrifices itself and protects the steel substrate. Ensure drainage so electrolyte doesn’t pool, and avoid the combination in aggressively marine settings without isolation.

What about 410 or 17-4 PH instead of 304/316?

Only when hardness or high strength is the limiting factor, not corrosion. 410 is hard but corrosion-limited; 17-4 PH reaches 1,300+ MPa tensile with better corrosion than 410. Neither replaces 316 for chloride service.

Is 316 always better than 304?

For chloride, marine, or chemical exposure — yes. For dry indoor or mild outdoor duty, 304 is fully sufficient and more cost-effective. “Better” depends on the environment, not the number.

What does the “л” mean in 316L?

“л” = low carbon (≤0.03%). It prevents sensitization during welding, keeping the weld zone corrosion-resistant. Always specify “л” grades for welded assemblies.

What is the difference between A2 and A4?

These are ISO 3506 property-class names: A2 = 304-type, A4 = 316-type. A4 adds molybdenum, so it resists chlorides that A2 cannot.

Why are my “stainless” bolts rusting?

Usually surface iron contamination, the wrong grade for the environment, or crevice corrosion. Passivation (ASTM A967) plus the correct grade resolves the issue.

Which grade is the strongest?

Among common grades, martensitic 410/431 (heat-treated) and duplex 2205 lead. Annealed 304 and 316 have similar moderate strength but gain substantially through cold working.

Stainless Steel Grades for Fasteners

Заключение

Choosing stainless steel grades for fasteners is less about memorizing alloy tables and more about answering one question well: what environment must this part survive? Map the environment, pick the family (304/A2 for benign, 316/A4 for chlorides, martensitic/PH/duplex for strength), confirm the property class for load, and respect the galvanic partner. Do those four things and most field failures disappear before they start.

The grade you specify is only as good as the process that makes it, so pair this knowledge with a supplier who controls wire, forming, heat treatment, and passivation at every checkpoint. To see how specification becomes a finished, documented part, explore our stainless steel fastener products, и keep our Ресурсы library handy.

Редакция Guxiang Metalwork

Более 12 лет в производстве крепежных изделий. Мы специализируемся на стандартных и нестандартных крепежных изделиях, гайках, пружинах и шайбах, включая холодную высадку, накатку резьбы, механическую обработку и штамповку. Наше предприятие соответствует стандарту ISO 9001. & Сертифицирован по стандарту IATF 16949 и предлагает услуги OEM/ODM по всему миру.

Оглавление

Отправить ваш запрос
Делиться:
Вам также может понравиться
семейство широкий_пластик_полимер
Материал изготовления крепежа – латунь
титановые крепления
Крепежные материалы
Hero_aluminum-крепежи
герой_аллой-стали-крепежи-2